1、Designation:D328917(Reapproved 2022)Standard Test Method forDensity of Semi-Solid and Solid Asphalt Materials(NickelCrucible Method)1This standard is issued under the fixed designation D3289;the number immediately following the designation indicates the year oforiginal adoption or,in the case of rev
2、ision,the year of last revision.A number in parentheses indicates the year of last reapproval.Asuperscript epsilon()indicates an editorial change since the last revision or reapproval.1.Scope1.1 This test method covers the determination of the densityof semi-solid and solid asphalt materials by weig
3、hing in air andin water.NOTE1An alternate method for determining the density of semi-solidand solid asphalt materials is Test Method D70/D70M.For materialswhich are too fluid for use of this method,use Test Method D3142/D3142M.1.2 The values stated in SI units are to be regarded as thestandard.No ot
4、her units of measurement are included in thisstandard.1.3 Warning Mercury has been designated by the UnitedStates Environmental ProtectionAgency(EPA)and many stateagencies as a hazardous material that can cause central nervoussystem,kidney,and liver damage.Mercury or its vapor may behazardous to hea
5、lth and corrosive to materials.Caution shouldbe taken when handling mercury and mercury-containingproducts.See the applicable product Safety Data Sheet(SDS)for details and EPAs websitewww.epa.gov/mercury/faq.htmfor additional information.Users should be awarethat selling mercury,mercury-containing p
6、roducts,or both,inyour state may be prohibited by state law.1.4 This standard does not purport to address all of thesafety concerns,if any,associated with its use.It is theresponsibility of the user of this standard to establish appro-priate safety,health,and environmental practices and deter-mine t
7、he applicability of regulatory limitations prior to use.1.5 This international standard was developed in accor-dance with internationally recognized principles on standard-ization established in the Decision on Principles for theDevelopment of International Standards,Guides and Recom-mendations issu
8、ed by the World Trade Organization TechnicalBarriers to Trade(TBT)Committee.2.Referenced Documents2.1 ASTM Standards:2C670 Practice for Preparing Precision and Bias Statementsfor Test Methods for Construction MaterialsD70/D70M Test Method for Specific Gravity and Density ofSemi-Solid Asphalt Binder(
9、Pycnometer Method)D140/D140M Practice for Sampling Asphalt MaterialsD3142/D3142M Test Method for Specific Gravity,APIGravity,or Density of Cutback Asphalts by HydrometerMethodD4311/D4311M Practice for Determining Asphalt VolumeCorrection to a Base TemperatureE1 Specification for ASTM Liquid-in-Glass
10、 Thermometers2.2 Other:CRC Handbook of Chemistry and Physics3.Terminology3.1 densitythe mass per unit volume of a material.3.2 relative densitythe ratio of the mass of a given volumeof a material to the mass of the same volume of water at thesame temperature(Note 2).NOTE2Relative density is also cal
11、led specific gravity.4.Summary of Test Method4.1 The sample is placed in a nickel crucible and weighed inair,and then in water at the test temperature.The density iscalculated from the mass of the sample and its apparent masswhen weighed in water.5.Significance and Use5.1 Values of density are used
12、for converting volumes tounits of mass,and for correcting measured volumes from thetemperature of measurement to a standard temperature usingPractice D4311/D4311M.6.Apparatus6.1 Crucible,nickel,high-form,approx.30 mL capacity,approx.43 mm in height by approx.41 mm in diameter.1This test method is un
13、der the jurisdiction of ASTM Committee D04 on Roadand Paving Materials and is the direct responsibility of Subcommittee D04.47 onMiscellaneous Asphalt Tests.Current edition approved Nov.1,2022.Published November 2022.Originallyapproved in 1974.Last previous edition approved in 2017 as D3289 17.DOI:1
14、0.1520/D3289-17R22.2For referenced ASTM standards,visit the ASTM website,www.astm.org,orcontact ASTM Customer Service at serviceastm.org.For Annual Book of ASTMStandards volume information,refer to the standards Document Summary page onthe ASTM website.Copyright ASTM International,100 Barr Harbor Dr
15、ive,PO Box C700,West Conshohocken,PA 19428-2959.United StatesThis international standard was developed in accordance with internationally recognized principles on standardization established in the Decision on Principles for theDevelopment of International Standards,Guides and Recommendations issued
16、 by the World Trade Organization Technical Barriers to Trade(TBT)Committee.16.2 Bath,constant-temperature,capable of maintaining thetest temperature within 60.1 C.6.3 Thermometric Device,calibrated liquid-in-glass,total-immersion type,of suitable range with graduations at leastevery 0.1 C and a maximum scale error 0.1 C as prescribedin Specification E1.Thermometer commonly used is 63C(63F).Any other thermometric device of equal accuracy maybe used.6.4 Balance,capable of weighing to 0.001 g.It sh