1、Designation:D148800(Reapproved 2013)Standard Test Method forAmylaceous Matter in Adhesives1This standard is issued under the fixed designation D1488;the number immediately following the designation indicates the year oforiginal adoption or,in the case of revision,the year of last revision.A number i
2、n parentheses indicates the year of last reapproval.Asuperscript epsilon()indicates an editorial change since the last revision or reapproval.This standard has been approved for use by agencies of the Department of Defense.1.Scope1.1 This test method covers the determination of the pres-ence or abse
3、nce of amylaceous(starch-like)material inphenol-,resorcinol-,and melamine-resin adhesives.1.2 The values stated in SI units are to be regarded as thestandard.The values given in parentheses are for informationonly.1.3 This standard does not purport to address all of thesafety concerns,if any,associa
4、ted with its use.It is theresponsibility of the user of this standard to establish appro-priate safety and health practices and determine the applica-bility of regulatory limitations prior to use.2.Referenced Documents2.1 ASTM Standards:2D907 Terminology of Adhesives3.Terminology3.1 DefinitionsMany
5、terms in this test method are definedin Terminology D907.4.Summary of Test Method4.1 A reagent solution is added to the adhesive in questionwhich causes any starch-like material to become insoluble.Theresultant material then changes color when another reagent isadded if any starch-like matter is pre
6、sent.5.Significance and Use5.1 This test method is used to determine if a melamineresin,a phenol,or a resorcinol adhesive contains any starch-like filler,the presence of which could affect water resistanceor strength,or both.6.Reagents6.1 Iodine Test SolutionAdd 5 g(0.18 oz)of iodine and 5g of potas
7、sium iodide to 100 mL(3 oz)of distilled water.6.2 Acetic AcidEthyl Alcohol SolutionAdd 20 parts ofglacial acetic acid and 20 parts of 95%ethyl alcohol to 60parts of distilled water by volume.7.Sampling7.1 Except in special cases,take a composite of the sampleof the adhesive when possible,from three
8、or more separatecontainers,chosen at random.Also,take samples from con-tainers that appear to be nonrepresentative,and test suchsamples separately.Before a sample is taken,thoroughly mixthe contents of the container if there is a tendency for thematerials to separate.Place the samples immediately in
9、 airtightcontainers and transport to the testing laboratory in thesecontainers.Take precautions to reduce evaporation or drying toa minimum.8.Procedure8.1 Phenol and Resorcinol AdhesivesWeigh 0.5 g(0.018oz)of thoroughly mixed adhesive into a small-diameter testtube.Add 5 mL(0.15 oz)of 95%ethyl alcoh
10、ol.Shakethoroughly,allow the insoluble matter to settle,and decant thesupernatant liquid.Repeat twice more with the ethyl alcoholand three times with distilled water.After the final decantation,add one drop of the iodine solution to the residue.A darkeningof the residue denotes a positive test for t
11、he presence ofamylaceous matter.8.2 Melamine ResinsUse the same procedure as specifiedin 8.1 except substitute an acetic acid-ethyl alcohol solution.When the melamine adhesive is supplied with separatehardener,use ethyl alcohol for the unmixed hardener.9.Report9.1 Report the following information:9.
12、1.1 Complete identification of the adhesive tested,includ-ing type,source,manufacturers code number,lot or batchnumber,condition,and date,and9.1.2 Positive or negative reaction to the iodine test.1This test method is under the jurisdiction of ASTM Committee D14 onAdhesives and is the direct responsi
13、bility of Subcommittee D14.30 on WoodAdhesivesCurrent edition approved May 1,2013.Published May 2013.Originallyapproved in 1957.Last previous edition approved in 2006 as D1488 00(2006).DOI:10.1520/D1488-00R13.2For referenced ASTM standards,visit the ASTM website,www.astm.org,orcontact ASTM Customer
14、Service at serviceastm.org.For Annual Book of ASTMStandards volume information,refer to the standards Document Summary page onthe ASTM website.Copyright ASTM International,100 Barr Harbor Drive,PO Box C700,West Conshohocken,PA 19428-2959.United States1 10.Precision and Bias10.1 No information is pre
15、sented about either the precisionor bias of Test Method D1488 for measuring the presence orabsence of amylaceous matter in adhesives since the result isnonquantitative.11.Keywords11.1 amylaceous matter;iodine test;melamine;phenol;resorcinol;starch-likeASTM International takes no position respecting
16、the validity of any patent rights asserted in connection with any item mentionedin this standard.Users of this standard are expressly advised that determination of the validity of any such patent rights,and the riskof infringement of such rights,are entirely their own responsibility.This standard is subject to revision at any time by the responsible technical committee and must be reviewed every five years andif not revised,either reapproved or withdrawn.Your comments are invited either for revi